Logo
Phthalogen Blue 3G ( Ingrain Blue 2.2 )
 Ingrain Brill Blue 3G Pdr. Dyeing for Fabrics
Padding Process :
4 Parts Ingrain Brill Blue 3G Pdr.
8 Parts Solvent Cum Emulsifier
10 Parts Urea
20 Parts Water followed by addition of
50 Parts Ice Cod Water & Add
8 Parts Copper Complex
100 Parts

Pad and dry the material at about 80-90 C.
Cure at 150 C for about 5 to 6 minutes.

After Treatment :
The material is rinse in cold water & is treated with Sodium nitrite 4 gms/litre & 5 gms/litre HCL at boil for 20 minutes. Wash with Soap and Soda ash at boil and rinse.

Ingrain Brill Blue 3G Pdr. Printing for Fabrics
Padding Process :
4 Parts Ingrain Brill Blue 3G Pdr.
10 Parts Urea
20 Parts Water
8 Parts Copper Complex after Stirring add
58 Parts Gum Thickening
100 Parts

Print on screen and dry in air. Steam for one hour wash with cold water and dry.